Jodhpur sandstone because of its strength, resistance to abrasion and aesthetic looks is one of the best sandstones of the world. Though sandstones of other regions such as Karauli, Dholpur,Banshi Paharpur and Bijolia are of the best quality Jodhpur sandstone stands almost at par as far as its chemical and physical properties are concerned.
Serial No. |
Stone Variety |
Compressive Strength N/mm2 (ASTM C-170) |
Water absortion, % by weight (ASTM C-97) |
Density(Bulk specific gravity) (ASTM C-97) |
Modulus of rupture, N/mm2 (ASTM C-99) |
Abrasion (Resistance to wear)(IS 1237 Guidelines) |
|
|
Dry |
Wet |
|
|
Dry |
Wet |
Average wear.mm |
Max. wear on indv. Sp ecimen .mm |
|
|
Para llel to rift |
Perpen dicular to rift |
Para llel to rift |
Perp en dicular to rift |
|
|
Para llel to rift |
Per pen dicular to rift |
Para llel to rift |
Perp en dicular to rift |
|
|
1. |
D.Beige |
115 |
108 |
106 |
91 |
1.82 |
2.36 |
16 |
9 |
13 |
8 |
2.9 |
3.1 |
2. |
Modak |
156 |
185 |
134 |
153 |
0.53 |
2.60 |
42 |
40 |
34 |
39 |
0.9 |
1.0 |
3. |
Jodhpur Red |
91 |
100 |
63 |
60 |
1.67 |
2.53 |
16 |
13 |
15 |
11 |
2.6 |
2.8 |
4. |
Jodhpur Pink |
93 |
72 |
63 |
48 |
2.21 |
2.40 |
18 |
16 |
18 |
16 |
2.4 |
2.7 |
5. |
Lalitpur Grey |
121 |
125 |
106 |
100 |
2.17 |
2.41 |
22 |
23 |
16 |
18 |
2.8 |
3.0 |
6. |
Lalitpur Yellow |
138 |
117 |
104 |
62 |
1.91 |
2.44 |
19 |
19 |
13 |
18 |
2.8 |
3.0 |
7. |
Bansi Pink |
84 |
74 |
50 |
54 |
3.52 |
2.28 |
11 |
13 |
9 |
10 |
4.2 |
4.4 |
8. |
Agra Red |
93 |
105 |
56 |
48 |
3.95 |
2.25 |
12 |
13 |
7 |
9 |
5.6 |
5.8 |
9. |
Teak Wood |
41 |
49 |
31 |
36 |
6.29 |
2.07 |
8 |
9 |
8 |
6 |
5.2 |
5.3 |
10. |
Rainbow |
63 |
61 |
27 |
20 |
5.00 |
2.11 |
11 |
9 |
10 |
7 |
5.2 |
5.4 |
Properties
Chemical Properties |
Percentage |
Physical Properties |
|
SiO2 |
96.60% |
Density kg/m3 |
2.42 |
Fe2O3 |
1.20% |
Water Absorption% |
1.25 |
Al2O3 |
1.00% |
Modulus of Rupture kg/cm2 |
222 |
CaO |
0.28% |
MgO |
0.20% |
L.O.I. |
0.50% |